Petroleum coke is a solid carbonaceous product obtained by high-temperature processing of heavy petroleum residues. It occupies an intermediate position between fuel products and special carbon materials, and its properties and applications are determined by structure and purity. By structure and purpose, two extreme types are distinguished — needle (anisotropic) and regular (isotropic or mosaic) coke, which differ both in production technology and in their performance characteristics.

Chemical Composition and General Properties

Petroleum coke consists predominantly of carbon. Depending on the feedstock and technology, the carbon content is 90–95%, hydrogen — no more than 1–2%, sulfur — from tenths of a percent to 3–8%, and nitrogen and oxygen compounds and ash elements (vanadium, nickel, iron, silicon) are also present. Raw (uncalcined) coke contains a significant amount of volatile matter (10–12%) and moisture (up to 12–18%), has a wide granulometric composition and is a dielectric. To impart electrical conductivity, density and mechanical strength, the coke is calcined at temperatures of 1200–1400 °C, which removes volatiles and forms an ordered carbon structure.

Needle Coke

Needle coke is a highly structured anisotropic carbon product with low metal and sulfur content. Its distinctive feature is a needle-like (fibrous) texture, which provides a high degree of orientation of carbon layers along the needle axis. This gives the material unique properties: a low coefficient of thermal expansion (CTE), high electrical conductivity, increased flexural strength and resistance to thermal shock.

The feedstock for needle coke production is low-sulfur cracking residues, deasphalted products and pre-aromatised heavy fractions. The process is carried out by delayed coking under strictly controlled temperature and pressure parameters, which allows an anisotropic structure to be formed. Key quality requirements for needle coke include low sulfur content (typically less than 1%), minimal ash, high true density after calcination and low CTE.

The main application of needle coke is the production of large-diameter graphite electrodes (500 mm and above) for electric arc furnaces, as well as ultra-high-power (UHP) electrodes. Such electrodes withstand extreme thermal loads and ensure stable arc discharge in steelmaking. In addition, needle coke is used for the manufacture of nipples (connecting elements for electrodes), in the nuclear, chemical and aerospace industries, and as a filler for special graphite materials. A growing area is the use of needle coke in the production of anodes for lithium-ion batteries, driven by the development of electric transport and energy storage systems.

Regular Coke

Regular (conventional) coke occupies an intermediate position between needle and isotropic coke. Its structure is less ordered, the sulfur and ash content is higher, and the CTE is greater. The feedstock for regular coke is cracked vacuum residues and fuel oils, as well as mixtures of thermal cracking residues with less valuable products.

Regular coke is produced mainly by delayed coking. Depending on the application, various requirements are imposed on it. For the production of anodes and anode mass for aluminium electrolysers, density, minimal ash content and granulometric composition are important. For graphite electrodes for electric steelmaking, sulfur content (no more than 1.0%), ash (no more than 0.6%) and true density after calcination are standardised.

The main applications of regular coke are the production of anodes for the aluminium industry, carbon electrodes, structural materials, and use as fuel in the cement, power and metallurgical industries. In metallurgy, coke is also used as a reducing agent. Part of regular coke is used to produce carbon black and in abrasive manufacturing.

Production Technology and Calcination

The basic industrial method for producing petroleum coke is delayed coking of heavy residues. The process includes heating the feedstock in a furnace, feeding it into coke drums, where at a temperature of 450–500 °C and a pressure of 0.3–0.5 MPa for 36–48 hours coke is formed, followed by cooling and extraction of the product. Needle coke requires more thorough feedstock preparation and control of coking conditions.

Calcination is a key stage of coke processing, carried out to increase density, electrical conductivity, mechanical strength and reduce reactivity. Calcination is carried out at temperatures of 1200–1400 °C for 60–90 minutes. The most stringent requirements for sulfur content and density apply to coke for graphite electrodes, which requires the use of low-sulfur feedstock and elevated calcination temperatures.

Market and Trends

Petroleum coke remains a large-tonnage product of global oil refining. The main consumers are the aluminium, steel and power industries. Regular (fuel-grade) coke dominates consumption, while needle coke occupies a niche but high-margin segment.

Key industry trends are linked to growing demand for high-quality carbon materials for electric steelmaking and lithium-ion batteries, tightening environmental requirements for emissions from fuel coke combustion, and the development of technologies to increase oil refining depth. The Asia-Pacific region remains the largest market for both production and consumption of coke.

Organising supplies of petroleum coke, including selecting the grade for a specific technology, logistics and financial support, requires an individual approach taking into account sulfur, ash and granulometry requirements.

Menu